Short answer: An electric arc furnace (EAF) magnesia-carbon (MgO-C) brick fails in four main ways: slag dissolves the magnesia, iron oxide in the slag burns the carbon, air and CO2 burn the carbon where slag does not cover the wall, and the brick loses carbon and strength through its own internal reactions at high temperature. Antioxidants such as aluminium, silicon, silicon carbide and boron carbide do not stop these attacks. They slow the carbon loss and help build a dense layer at the hot face. The right mix depends on the zone of the furnace, so a brick for the slag line should not be copied for the hot spot or the lower sidewall. To compare suppliers, ask for the brick design by zone, a cut-face report of a used brick, and the cost per tonne of steel, not the price per brick.
1. Why This White Paper Exists
Magnesia-carbon bricks were first developed for the hot spots of electric arc furnaces, and only later moved to converters in the late 1970s. So the EAF is where this material has the longest history. It is also where purchasing and engineering teams still argue the most about it: Is a higher graphite brick better? Is boron carbide worth the price? Why did the same brand last twice as long in the neighbouring furnace?
We make refractories, so we have a view. We also try to say which statements come from published work and which are our own reading. Where we have no solid number, we say so and we do not invent one.
In this paper you will find:
- The four ways an EAF MgO-C brick wears, in plain language;
- What each antioxidant does, and where it can cause trouble;
- How to tailor a brick to each zone of the furnace;
- How to read a used brick, and what to send a supplier;
- A cost per tonne method, and 18 questions with direct answers.
2. How an EAF Magnesia-Carbon Brick Is Built
Three jobs, three ingredients
A MgO-C brick is a team of materials, and each does one job.
- Magnesia grains resist slag and heat. They make up most of the brick.
- Graphite is not wetted by slag, conducts heat well and expands little. That keeps slag out and helps the brick survive heating and cooling.
- A carbon bond (usually resin) holds the brick together and leaves a carbon network after the first heat-up.
The problem is that graphite burns. Everything else in this paper follows from that.
Ranges quoted in the literature
| Item | Typical range | Note |
|---|---|---|
| Carbon content of MgO-C bricks | 8% to 30%, most common 10% to 20% | A published steelmaking reference |
| Antioxidant additions | About 2% to 3% in total | Aluminium and silicon are the most common |
| Graphite in intermittently run EAFs | Often higher | Where heating and cooling are more frequent |
| Service temperature | Above 1,500 °C | Refining slag can exceed 1,650 °C |
| Coarse aggregate | 1 to 7 mm, about 70% of the brick | Matrix is finer, 50 to 500 µm |
These are general figures from published reviews, not a specification for any one furnace. Your own numbers should come from your supplier’s data sheet and your own furnace.
Fused or sintered magnesia?
One published reference table compares one fused sea-water magnesia (99.07% MgO, 2.6% apparent porosity) with one natural sintered magnesia (95.46% MgO, 8% apparent porosity). That is a single example, not a rule. But it shows the direction: fused grains tend to be purer and denser, so slag finds fewer paths into them. Impurities such as SiO2 and CaO in the grain matter because they form low-melting phases with iron oxide.
In our view, the grain choice should follow the zone. We come back to this in the zone table.
3. The Four Ways an EAF MgO-C Brick Wears
1. Slag dissolves the magnesia
Slag attacks the magnesia in two ways. Silica and lime enter the boundaries between grains and loosen them. Iron oxide (FeO) diffuses into the magnesia grain itself and forms a magnesia-iron oxide solid solution, which melts at a lower temperature than pure magnesia.
A laboratory study at 1,600 °C with 25% FeO slag found the most severe wear at a basicity of 0.5, and little wear from about 2.0 upward. Furnace practice and slag chemistry therefore matter as much as the brick. A brick that does well with a basic, MgO-saturated slag can suffer badly when slag turns acidic.
2. Iron oxide burns the carbon from inside
When slag gets into the brick, iron oxide meets graphite and the reaction FeO + C → Fe + CO takes the carbon away. The brick turns porous and weak, more slag enters, and the loss speeds up. A published review names this reaction as the cause of structural embrittlement in the brick.
3. Air and CO2 burn the carbon where the slag does not cover
The hot face of an EAF wall is not always under slag. Where the brick sees furnace air or CO2, carbon burns directly. Published work places direct oxidation below roughly 1,400 °C, and indirect oxidation by magnesia or slag above it. This is why lower sidewalls and areas that are often uncovered need oxidation resistance, even where slag attack is mild.
4. The brick attacks itself
At high temperature, magnesia and carbon can react: MgO + C → Mg(gas) + CO(gas). Under standard conditions the reaction starts at about 1,850 °C. In a real brick the gas can escape through pores, so it can run at a much lower temperature. The brick loses material from inside, and the result is a weak, open structure. Published tests also report that cutting very fine magnesia (0.1 mm and finer) reduces this kind of damage.
Thermal cycling and mechanical wear
On top of these four, an EAF brick is heated and cooled again and again, hit by scrap, and washed by moving steel. Heating cycles loosen the structure over time. A published converter study found that repeated heating above 1,500 °C and cooling below 500 °C could reproduce real brick damage in the laboratory. Wear by moving steel falls as the brick’s hot strength rises.
Why they feed each other
The four mechanisms rarely act alone. Carbon loss opens pores. Open pores let slag in. Slag brings more FeO. More FeO burns more carbon. If you remember one thing from this section, let it be this: a brick usually dies from a loop, not from one cause. Break the loop at its weakest link, and the whole brick lasts longer.
4. Where in the Furnace the Brick Fails
In many furnaces the upper wall uses water-cooled panels, so bricks work mostly in the lower shell, the slag line and the hot spots. Layouts differ, so check yours.
| Zone | Main threat | What it looks like in a used brick |
|---|---|---|
| Hot spot (nearest the arcs) | Very high temperature, arc radiation, fast slag attack | Thin remaining brick, glazed or washed hot face |
| Slag line | Slag attack and FeO, changing slag level | A groove at the slag level |
| Sidewall above or below the slag | Air and CO2 oxidation, thermal cycling | A deep decarburized layer, cracks parallel to the face |
| Charging side (scrap impact) | Scrap impact, heating and cooling | Chipped or spalled faces |
| Tap area | Flow of steel, repeated heating, oxidation | Eroded bore, cracks |
The exact order of wear depends on your furnace design, power input, slag practice and scrap mix. We do not give a general life figure. If someone gives you one without conditions, treat it with care.
5. What Antioxidants Do, and What They Cannot Do
An antioxidant is a material that is more eager to react with oxygen than graphite is, or that blocks the path of oxygen into the brick. It protects the carbon, but it does not make a poor brick good.
Aluminium
Aluminium reacts with carbon monoxide and carbon in the brick. A published laboratory study with an argon atmosphere found a liquid containing aluminium and magnesium at low temperature, then, after about 850 °C, aluminium carbide as thin platelets. Above 1,000 °C the aluminium carbide reacts with magnesia to form magnesium aluminate spinel (MgAl2O4), which sits well beside both magnesia and carbon. The overall effect is to fill pores and slow oxygen.
Watch-out (our practice note): aluminium carbide can react with moisture. Keep bricks dry in storage and during transport.
Silicon
Silicon reacts with carbon to form silicon carbide (Si + C → SiC). The new SiC fills pores and protects graphite. It is often paired with aluminium. Published reviews note that aluminium and silicon are the most used antioxidants because they are effective and low in cost.
Silicon carbide (added as SiC)
SiC added as a powder acts in two ways. It resists oxidation itself, and it fills pores. Published converter practice adds SiC to the throat and cone, where gas-phase oxidation is a problem. The same logic suits furnace walls that are often uncovered by slag.
Boron carbide
Boron carbide reacts with carbon monoxide and forms liquid boron oxide, which combines with magnesia to give a liquid MgO-B2O3 phase. In published reviews this liquid fills pores at medium temperatures and limits air access. That is its strength.
Watch-out (our reading, not a published figure): a liquid phase can soften a brick when the face is very hot. We would check it carefully before using boron carbide in the hottest zones, and we would ask the supplier for hot strength data.
What antioxidants cannot do
- They do not stop slag from dissolving magnesia. For that, you need pure, dense grains and a sound slag practice.
- They do not cure a bad heat-up. A wet or fast-heated brick will crack, whatever is in it.
- More is not always better. An antioxidant that reacts too early or leaves a weak phase can cost you hot strength. The overall design matters more than one additive.
6. Tailoring the Brick to the Zone
There is no single best EAF brick. There is a best brick for each zone of your furnace, built from your slag, your scrap and your practice.
| Zone | Magnesia grain | Carbon | Antioxidant direction (to be tuned) | Why |
|---|---|---|---|---|
| Hot spot | High-purity fused magnesia, low impurity | Enough graphite for thermal shock, purity matters | Aluminium and silicon based, check any boron carbide with care | Highest temperature and fast slag attack |
| Slag line | High-purity fused magnesia, dense | Mid to high, well protected | Aluminium and silicon, SiC where FeO is high | FeO attack and the level changes |
| Lower sidewall | Good quality fused or high-grade sintered | Mid, with strong oxidation protection | Aluminium and silicon, SiC, boron carbide can help at medium temperatures | Air and CO2 reach the brick |
| Charging side (scrap impact) | Strong, tough matrix | Higher graphite helps with thermal shock | Metals that add strength | Impact and thermal shock |
| Tap area | Dense, high purity, shaped to drawing | Mid | Matched to the flow and heat cycle | Steel flow and heat cycles |
“Mid” and “higher” mean relative levels inside your own range of bricks. We do not give fixed percentages, because the right figure depends on the furnace and the supplier’s recipe.
Three trade-offs worth knowing
- Higher graphite lowers thermal shock risk but also gives the oxidation more to burn. More carbon needs better protection, not just more of it.
- Purer magnesia costs more but often pays back in the hot spot and slag line, where slag attack drives the loss. In the sidewall, the saving may not be worth it.
- Metal antioxidants strengthen the brick but can raise cost and handling needs. Use them where they work, not everywhere.
What a custom design needs from you
The more of this you send, the closer the first design will be:
- furnace type, capacity, power and tap-to-tap time;
- lining drawing and brick thickness by zone;
- scrap mix and any direct-reduced iron or hot metal;
- slag practice (basicity, MgO addition, foaming, FeO range);
- current brick, life in heats and how it fails, by zone;
- photos of used bricks and of the furnace in service.
7. Reading a Used Brick: 4-Step Analysis
A used brick is a free test report. Here is how to read it.
Step 1. Photograph the hot face first
Take photos before you cut or clean the brick. Note the zone, the position and the heat count.
Step 2. Cut through the thickness
Cut from the hot face to the cold face and look at the cut surface.
Step 3. Measure the layers
Record the thickness of each layer from the hot face, in millimetres: slag-covered layer, dense layer, carbon-free layer, unaffected core.
Step 4. Decide
| What you see | Likely meaning | What we would look at |
|---|---|---|
| Thick, porous carbon-free layer | Oxidation is the main cause | Antioxidant system, storage and heat-up, slag cover |
| Slag deep inside, grains rounded | Slag attack is the main cause | Magnesia purity and density, slag basicity and FeO |
| A dense, thin layer at the hot face | A protective layer formed and held | Keep the recipe, check heat-up and practice stay stable |
| Cracks parallel to the hot face | Thermal cycling or fast heat-up | Graphite level, heat-up curve, power-on practice |
| Wear groove at slag level | Slag-line attack with changing level | Brick grade at that line, slag level control |
| Fine white deposit on the cold face | Magnesium vapour escaping and re-oxidising (published lab work reports MgO whiskers on the cold face) | Our reading: check density and carbon balance |
What the tests can add
Start with simple tools
Photos, a ruler and an optical microscope tell you a lot. Bulk density and apparent porosity of an unused brick come from standard tests.
Then add instruments when you need them
A scanning electron microscope with element analysis (SEM/EDS) shows which phase holds which element. X-ray diffraction (XRD) names the crystal phases, for example spinel or silicon carbide.
Do not over-read one brick
One brick can mislead. Compare it with an unused brick from the same batch, and with another used brick from the same zone.
8. Counting the Cost per Tonne of Steel
A brick that costs less but lasts fewer heats can cost more per tonne.
Lining cost per tonne = (brick price + installation + repair and downtime cost) / (heats × tonnes per heat)
An example with made-up numbers, for illustration only:
| Parameter | Brick A | Brick B |
|---|---|---|
| Lining cost for the zone (units) | 1,000 | 1,350 |
| Heats achieved | 400 | 650 |
| Tonnes per heat | 100 | 100 |
| Cost per tonne (units) | 0.025 | 0.021 |
In this made-up case the dearer brick wins. Add two more lines from your own records: the cost of one unplanned stop, and any extra repair of that zone. An unplanned stop can cost more than the bricks.
9. Six Checks Before You Order
| Ask | Why | A good answer sounds like |
|---|---|---|
| Is the brick designed by zone? | One brick cannot suit every zone | A list of grades by zone with the reason |
| What is the magnesia grain and its MgO, SiO2 and CaO? | Impurities lower the melting point | Numbers from the data sheet, with the test method |
| Which antioxidants, and what is the logic? | To avoid copied recipes | A reason tied to your zone and slag |
| How does it behave in an oxidation test? | To see the carbon loss in a repeatable test | A test result with method and conditions |
| Can I see the cut face of a used brick? | The real test report | Photos and layer depths in millimetres |
| How many heats on a similar furnace? | To set a realistic target | A range with conditions, not one perfect number |
10. How YK Chanshine Works with EAF Teams
We make magnesia-carbon bricks and other refractories for steel plants. Our process on an EAF project is simple:
- You send furnace data, slag practice and photos of used bricks.
- We read the wear pattern with you, by zone.
- We propose a brick design for each zone and say what we would change and why.
- We put the storage, installation and heat-up notes in writing.
- After the trial we read the used bricks together, and adjust.
11. Frequently Asked Questions (FAQ)
What are magnesia-carbon bricks used for in an electric arc furnace?
They line the parts of the furnace that meet the hardest conditions: hot spots near the arcs, the slag line, and parts of the lower sidewall. They combine the slag resistance of magnesia with the heat conduction and slag-repelling nature of graphite.
Why do EAF MgO-C bricks wear out?
Four main reasons: slag dissolves the magnesia, iron oxide burns the carbon from within, air and CO2 burn the carbon where slag does not cover the wall, and the brick can react with itself at high temperature. Heating cycles and scrap impact add to the damage.
How much carbon should an EAF brick have?
Published reviews give a wide range, from about 8% to 30%, with 10% to 20% most common. Higher carbon helps with thermal shock but needs better oxidation protection. The right level depends on the zone and your practice, so ask for the design logic, not just a number.
What is the role of antioxidants in MgO-C bricks?
They protect the carbon. Metals such as aluminium and silicon, and compounds such as boron carbide, react with oxygen or carbon monoxide and form products that fill pores and slow oxygen. They do not stop slag from dissolving magnesia.
What does aluminium do in a MgO-C brick?
Aluminium reacts with carbon and gas in the brick to form aluminium carbide. Above about 1,000 °C, the carbide reacts with magnesia to form spinel. The spinel and the other products fill pores. Keep the bricks dry, because aluminium carbide can react with moisture.
What does silicon do in a MgO-C brick?
Silicon reacts with carbon to form silicon carbide, which fills pores and protects the graphite. Silicon is widely used with aluminium because it works well and costs less than many alternatives.
Is boron carbide worth the extra cost?
It can be, in zones where air reaches the brick at medium temperatures, because it forms a liquid phase that seals pores. In the very hottest zones, a liquid phase might soften the brick, so ask the supplier for hot strength data and a used-brick report.
What is a decarburized layer?
It is the layer of a used brick where the carbon has burned out. It is porous and weak, so slag can enter and the layer can peel away. Its thickness in millimetres, measured from the hot face, is one of the most useful numbers from a used brick.
What is a dense layer at the hot face of a used brick?
At high temperature, a dense layer of magnesia, or magnesia with spinel, can form at the hot face. It slows further oxidation and slag entry. If your used bricks show this layer and it stays in place, your recipe and practice are probably working together.
Should I choose fused or sintered magnesia for an EAF brick?
Fused magnesia is usually purer and denser, and often suits the hot spot and slag line. Good sintered grades can be enough for less severe zones. Check MgO, SiO2, CaO and porosity on the data sheet, and compare cost per tonne, not price per brick.
How does slag basicity affect brick wear?
A laboratory study at 1,600 °C with 25% FeO found the worst wear at low basicity (0.5) and very little wear from about 2.0 upward. Real furnaces are more complex, but the message is clear: slag practice and brick choice must be set together.
Why does the same brick last longer in one furnace than in another?
Furnace design, power input, scrap mix, slag practice, heat-up routine and tap-to-tap time all change how much work the brick has to do. Compare furnaces with the same conditions, or ask your supplier to show the conditions behind any life figure.
How should MgO-C bricks be stored?
Keep them dry and off the floor, protected from rain and humid air. Moisture can harm the resin bond and some antioxidants. Check the packaging on arrival, and do not stack beyond what the pallet is made for.
How should a new EAF lining be heated up?
Follow the supplier’s written heat-up curve and keep the slow hold at low temperature so volatiles can leave. Heating too fast can cause cracks and spalling. A bad first heat-up can undo a good recipe.
How do I know if oxidation or slag attack is the main wear cause?
Cut a used brick and measure the layers. A thick, porous, carbon-free layer points to oxidation. Slag deep inside the brick with rounded grains points to slag attack. Often you see both, and the measured depths show which one leads.
Can you tailor a MgO-C brick to my furnace?
Yes. Send the furnace type and capacity, lining drawing, slag practice, scrap mix, current brick and its life by zone, and photos of used bricks. We reply with a zone-by-zone proposal and the reasons.
What should I send for a technical review or quote?
Send furnace data, the lining drawing by zone, slag practice, current brick and life in heats, photos of used bricks, and the target you want to reach. Photos of a cut face with a ruler are very helpful.
How do I calculate the cost per tonne of an EAF lining?
Add brick price, installation and repair or downtime cost for the zone, then divide by heats times tonnes per heat. Use your own records for stoppage cost. A dearer brick that runs longer often costs less per tonne.
12. Reference Sources
The published facts in this paper come from the following. Our own judgements are marked as such in the text.
- Magnesia-Carbon Refractories, Ispatguru
- Magnesia-Carbon Refractories for Converters, Nippon Steel Technical Report No. 125, 2020
- Reaction Chemistry and Microstructure Development of MgO-C Refractories Containing Metal Antioxidants, Guha and Smith, 2006
- The influence of slag basicity and composition on ConArc magnesia-carbon refractories during the blowing phase, A. Muller, Journal of the Southern African Institute of Mining and Metallurgy, 2011
13. Talk to Us About Your EAF Lining
Tell us your furnace data, slag practice and the current brick with its life by zone. We reply with a technical view.
Email: sales@ykchanshine.com | WhatsApp: +86 139 9807 2158 | Online Inquiry: Contact Us