Tundish Dry Vibration Mix vs Board vs Coating | YK Chanshine

Tundish Dry Vibration Mix vs Board vs Coating | YK Chanshine

By Jack Xing, Technical Sales Director, YK Chanshine · Continuous Casting Refractories · Updated

Tundish lining guide cover: insulation board, spray coating and dry vibration mix compared for continuous casting
Tundish lining guide cover

A tundish lining decides three things at once. It decides how clean your steel stays between ladle and mold. It decides how long your sequence can run before the tundish has to come off the car. And it decides how much gas, labor and turnaround time your prep bay spends between casts.

Most continuous casting shops use one of three working-lining systems: insulation boards, spray / trowel coatings, or a dry vibration mix. This guide compares their chemistry, operating trade-offs, binder choices and installation discipline, with typical TDS ranges and a checklist for quoting.

Key points from this guide:

  • Dry vibration mix delivers the longest sequence life (20 to 60+ hours) and cleanest steel because it brings zero free water and forms a dense hot face with an insulating backing.
  • Insulation boards require no pre-heat equipment and deskull easily, but silica boards can react with Al-killed steel, causing inclusion defects.
  • Spray coatings sit between the two on material cost, but require long, high-temperature gas baking (800–1000 °C) to drive out water.
  • Ultra-low-carbon and hydrogen-sensitive grades require inorganic binders (polyphosphate, sodium silicate, or boric acid) to eliminate carbon and hydrogen pickup.

At a glance: board vs. coating vs. dry vibration mix

Tundish working-lining systems compared
Question Board Spray / trowel coating Dry vibration mix
Water in the system None High None
Pre-heat Cold start possible 800–1000 °C, 2–6 h 200–300 °C, 45–90 min (or quick-heat)
Strongest point Fast, easy tear-out Low cost to apply, good insulation Long life, dense hot face, clean steel
Main risk Si, H or strength problems, depending on type Water attack, H and O pick-up, spalling Needs former and discipline
Typical life Short sequences Longer than board 20 h+, 60–70 h reported
Comparison of tundish working lining systems: insulation board, spray coating and dry vibration mix
Comparison of tundish working lining systems

The tundish lining: zones and layers

A continuous casting tundish has several refractory zones, each with its own role:

Cutaway of a continuous casting tundish showing steel shell, insulation, permanent lining, working lining, dam, weir and gas curtain
Cutaway of a continuous casting tundish
  • Insulating layer: sits against the steel shell (calcium silicate board or ceramic fiber) to protect the shell from overheating.
  • Permanent (safety) lining: high-alumina bricks or low-cement castable that remains in place for months.
  • Working lining: the replaceable layer (board, spray or dry mix) in direct contact with molten steel and tundish slag.
  • Flow control furniture: impact pad, weirs, dams and turbulence inhibitors that govern residence time and inclusion flotation.

Insulation boards

Tundish boards are pre-formed panels wedged or mortared against the permanent lining. They allow cold starts and very fast deskulling, making them popular for small billet casters running short sequences.

Tundish insulation board selector: silica, magnesia and forsterite board matched to steel grade
Tundish insulation board selector
Board types compared
Board Best for How it performs Watch-out
Silica board Plain carbon & rebar Low cost, easy install SiO₂ reduces in Al-killed steel, causing inclusions
Magnesia board Clean & alloy steel High basicity, low reaction Needs careful storage to avoid hydration
Forsterite board Intermediate grades Balanced thermal expansion Lower refractoriness than pure MgO

Spray and trowel coatings

Coating mixes are applied with robotic spray arms or trowels. While cheaper per ton than dry mix, they introduce 15% to 25% water that must be completely removed by gas baking:

Spray coating operating window
Parameter Typical range Impact on caster
Water addition 18–25% (spray) / 14–18% (trowel) High hydrogen risk if pre-heat is shortened
Bake-out cycle 800–1000 °C for 2–6 hours Consumes significant fuel gas in prep bay
Rebound loss 5–12% during application Material waste during spraying

Dry vibration mix

Dry vibration mixes (MgO 80% to 92%) represent the current standard for clean steel and high-productivity sequence casting. Because they are installed completely dry around a heated former, there is no water to drive off.

Organic vs inorganic binder for tundish dry vibration mix: carbon, hydrogen, fume and strength comparison
Organic vs inorganic binder for tundish dry vibration mix
Organic vs. inorganic binders for dry mix
Binder type Common materials Advantages Limitations
Organic Phenolic resin, novolac, pitch High green strength after bake at 200–250 °C Emits smoke/fumes during cure; adds C and H
Inorganic Polyphosphate, sodium silicate, boric acid Zero smoke, zero carbon/hydrogen pick-up Requires strict former temperature control
Nine-step installation sequence for tundish dry vibration mix: former, vibration, curing, stripping and firing
Installation sequence for tundish dry vibration mix

Typical TDS specifications for dry vibration mix

Dry vibration mix TDS benchmarks
Parameter Standard grade (billet) High-purity grade (slab / clean steel)
MgO content (%) 82.0–85.0% 88.0–92.0%
SiO₂ content (%) ≤ 5.5% ≤ 3.0%
CaO content (%) ≤ 3.0% ≤ 2.2%
Bulk density (g/cm³) 2.10–2.25 2.25–2.40
Cold crushing strength (after cure 250 °C) ≥ 4.0 MPa ≥ 5.0 MPa
Cold crushing strength (after firing 1500 °C) ≥ 18.0 MPa ≥ 25.0 MPa

Tundish furniture & flow modifiers

Tundish dam, weir and gas curtain flow control diagram showing how inclusions float out of the steel
Tundish dam, weir and gas curtain flow control diagram

Precast dams, weirs, and turbostops work in tandem with the dry vibration mix to optimize fluid flow, extend residence time, and prevent short-circuiting to the metering nozzle.

Flow control shapes compared
Shape Location Main function
Turbostop / impact pad Directly below ladle shroud Dissipates kinetic stream energy, prevents slag vortexing
Weir Between pouring & casting zones Forces steel flow downward, retains top slag
Dam Ahead of strand nozzle Forces steel flow upward to promote inclusion float-out

Decision guide: choosing the right lining for your caster

Lining choice by caster configuration
Caster type Steel grades Recommended working lining
Small billet caster (short sequences < 4 heats) Rebar, merchant bar Silica or low-MgO insulation board
Medium billet / bloom caster (4–12 heats) Structural, SBQ carbon MgO spray coating or 82% MgO dry mix
High-production slab caster (10–30+ heats) Deep drawing, IF steel, API linepipe High-purity MgO dry vibration mix (88–92% MgO)
Ultra-low-carbon / bearing steel caster 100Cr6, tyre cord, ULC Inorganic-bonded high-purity MgO dry mix

Frequently Asked Questions (FAQ): Tundish Working Lining Systems

What is the difference between a tundish dry vibration mix and a coating?

A coating is mixed with water and applied wet, so it needs a long bake at 800–1000 °C. A dry vibration mix is placed dry, vibrated around a former and cured at only 200–300 °C, so it brings no free water into the lining.

How long does a tundish dry vibration mix last?

Typically 20 casting hours or more. High-end results of 60–70 h are reported. Actual life depends on steel grade, slag, temperature and installation quality.

Can I use silica board for Al-killed steel?

It is not recommended. Al and Mn in the steel reduce the SiO₂ in the board, forming Al₂O₃ and 2MnO·SiO₂ that add oxide inclusions.

Which binder is best for ultra-low-carbon steel?

An inorganic binder such as polyphosphate, solid sodium silicate or boric acid. It adds no carbon or hydrogen and gives off no irritating fumes during cure.

What temperature do I cure a tundish dry mix at?

Heat the former to 200–300 °C for 1–2 h, strip it, then fire for about 1 h to above 1000 °C before use. Always follow the supplier’s own guide.

Why do tundish dams and weirs use magnesia?

Magnesia keeps its strength in steel, costs less than alumina-magnesia, and absorbs Al₂O₃ inclusions to form a spinel skin. It is also reported to carry about 80% less oxygen into the steel than high-alumina furniture.

Why add α-Al₂O₃ and silica microfines to a dam castable?

Alumina microfines react with MgO to form spinel with about 8% expansion, which densifies the matrix. Silica microfines reduce hydration and cracking but create low-melting phases, so they are kept at about 2% or below.

What should I send to get a tundish lining quotation?

Capacity, strand count, steel grades, sequence length, slag data, current lining and failure mode, binder restrictions, quantity and port. We reply with a grade recommendation and the TDS.

Send Us Your Continuous Caster Parameters & Sequence Targets

Looking to extend sequence casting hours, reduce turnaround downtime, or eliminate hydrogen/oxygen pick-up in clean steel? Send us your caster format (billet/bloom/slab), steel grades, sequence length, and current lining life. We provide custom dry mix / board recommendations, TDS, and cost comparisons within 24 to 48 hours.